Alpha Horizontal Centrifugal Casting Machines

Fault Possible Cause
a Lapping Pouring too slow Metal not hot enough
b Tube outer dia. rough Protrusion of pouring bucketspout in bore beyond the end plate of mould
c Slag/oxide bands produced Inadequate deoxidizing agent in ladle
d Bore tube oxidization Temperature of metal too low. Mould temperature too low. Crucible/pouring bucket temperature too low. Furnace and casting pouring into mould delayed.
e Rough tube surface at spray end Mould not cool enough. Spinning time of mould insufficient to cool mould
f Tube surface dimpled often at center Low spin speed. Pressure of spray tank too high. Low metal temperature. Consistancy of mould wash too smooth.
g Tube length incomplete or tapered tube wall Mould contains refractory material, possibly from pouring bucket or furnace. Pouring bucket or sprout requires maintenance.
h Spray end showing isolated patches of slag Belling at either or both ends of tube. Check dimensions of mould. Check coating. Check mould temperature.
i Casting difficult to remove Belling at either or both ends of tube. Check dimensions of mould. Check coating. Check mould temperature.
j Tube surface inconsistent (a spiral appearance may be produced) Inadequate mould coating in tank. Spray cone nozzle worn or restricted. Coating slurry too thin.
k Large diameter tubes longitudinal cracks in casting Tube run on at high speed for too long after casting.
l Surface of tube covered with pin holes, especially pronounced at spray end Low metal temperature. Oil traces in airline (faulty liner).
m Cracking/tearing fracture around circumference Contraction of tube restricted. Mould wash left in mould, inadequate cleaning Belling - refer to i.
n Patches of slag deposits on spray end of tube Metal deposits require cleaning at furnace and/or ladle.
o Pin-holing in patches and/or condensation Lance dripping with spray or craters at spray end. Lance sloping downwards.
p Molten metal raining in mould Molten metal temperature too high. Speed too low.

Gibson Centri Tech Ltd

Centrifugal Casting Machine Suppliers and Manufacturers

Email

sales@gibsoncentrich.co.uk

Phone Number

00 44(0)1543 418701

Business Hours

Monday to Thursday 8.30am – 5.00pm
Friday 9.00am – 4.00pm

Gibson Centri Tech Ltd

Hilltop Works
Trent Valley Industrial Estate
Eastern Avenue
Lichfield
Staffordshire
WS13 6UY